Basics of EBSD
Calibrating
the EBSD system
EBSD system calibration measures
the sample to screen distance and the pattern centre position on the
phosphor screen (Figure 5). The pattern centre is the point on the screen
closest to the generation point of the diffraction pattern on the sample.
There are several methods for calibrating an EBSD system.
One method to measure the pattern
centre position is to collect a diffraction pattern with the screen both in
the normal and partly retracted position and to measure the positions of the
same zone axes on both patterns (Figure 7). The screen to sample distance is
calculated by measuring the distance between two zones separated by a known
angle with the screen in the operating position. The calibration can also be
performed using a single pattern by iteratively fitting the pattern centre
and sample to screen distance to minimise the error in the
orientation
measurement